HOME > Product > Liquidity

Liquidity

Name : WINFLOW-SP||(High-strength and high-liquidity concrete)

Type : Standard Type

Download : 다운로드

WINFLOW-SP[Ⅱ]    High-strength and high-liquidity concrete

High-strengthand high-liquidity concrete use naphthalene sulfonic acid condensates as themain ingredient. It strongly disperses the cement particles so that it can makeconcrete with excellent fluidity at the low water/cement ratio. In addition,while preserving the properties of the base of the concrete, concrete can bepoured easily as its fluidity improves.

USAGE 

* Whenmanufacturing high-strength concrete and mortar
*
Whenmanufacturing fluidity concrete
*
Concretesecondary products (files, Hume, electric pole, segment, etc.)
*
Whenmanufacturing P.C concrete
*
Forself-leveling and special cement

 

DOSAGE
*
Typicalratios of 0.3% to 2.0% byweight of cement are suggested. Please test concrete to make sure each batchmeets the exact specification on site.

* Afteradding it, the mixture is mixed for 2-3 minutes at the high-speed rotation andthen concrete is placed.

* Afteradding it 0.1% to concrete, an standard increase in slump is 2±0.5.

* Excessivecement in concrete can lead to the decrease in bleeding, segregation, and theamount of air.

 

ADVANTAGES

* Concreteplacing can be easy when the liquidity is enhanced.

* Itincreases the durability.

* Itenhances the ability to pump.

* Sincethe condensation delay is little, air can be reduced.

* Aggregationof the cement particles is inhibited and its surface is smooth with theexcellent dispersion.

* Sincethere is no chloride, there is no promotion action on rebar corrosion

 

PROPERTIES

* Appearance  : Light  brown liquid

* Specific gravity   : 1.200±0.05 (20℃)

* pH       :  7.0±3.0

* Mainingredient: Naphthalene condensates

 

 

Packing : 10kg, 250kg/drum, Tank Lorry

MixingDesign

 

Class

 Mixing

 W/C(%)

S/A(%)

 W (㎏/㎥)

 C (㎏/㎥)

 AD (CXwt%)

 1

 BASE CONCRETE

58.4

 46.0

187

320

-

 1-1

 WINFLOW-SP [Ⅱ]

0.5

 2

 BASE CONCRETE

 60.0

 47.0

 192

320

 -

 2-1

 WINFLOW-SP [Ⅱ]

0.5

 3

 BASE CONCRETE

 61.3

 48.0

 196

320

 -

 3-1

 WINFLOW-SP [Ⅱ]

 0.5

 

 

 

 

TestResults


 

Test Item

 SLUMP (㎝)

 AIR (%)

 AIR

 Compressive strength  (MPa)

 Initial

 Final

 3Day

 7Day

 28Day

1

 8.0

1.5

 7;15

 9:15

  11.5

  19.0

 27.5

 1-1

 18.5

1.2

7:40

 9:25

 12.0

 19.8

 27.7

 2

 10.5

1.6

7:20

 9:25

 10.5

 18.6

 24.0

2-1

20.5

1.2

7:50

 9:30

 10.5

 18.8

 24.4

 3

12.0

1.5

7:40 

 9:45

 9.5

 16.2

 21.7

 3-1

 22.0

1.1

8:20

 9:40

 9.9

 16.3

 21.9

 